The Journal: The Cyano Codex blog · No. 3

Cyanotype under the microscope: blue particles in the fiber

A cyanotype has no binder, and yet the blue doesn’t come off on your fingers. A team at Tokyo University of the Arts looked very closely, down to the particles, at where Prussian blue lodges in the paper. What they saw, what they still don’t know and what it changes for anyone who washes or stores their prints.
Published
Reviewed
Reading time
7 min
Sources
5

As an Amazon Associate I earn from qualifying purchases. How we fund the site

In short

  • In cyanotype, Prussian blue also forms inside the cotton fibers, not just on top.
  • The particles measure about 20-100 nm on the fiber surface and 20-50 nm inside it.
  • That is why the solution should soak the paper, and why old prints are not cleaned with water.
On this page (7 sections)
  1. How does a blue stay put without a binder?
  2. The experiment
  3. What they saw: blue inside the fiber
  4. Particles that grow with light
  5. What does this mean for washing a cyanotype?
  6. And for preserving it?
  7. What is still unknown

How does a blue stay put without a binder?#

The blue of a cyanotype holds to the paper without a binder because it forms inside it. The traditional recipe has no binder, and even so your hands don’t get stained when you touch a dry print, and not all the blue goes in the wash1. A 2025 study set out to see why.

That “inside” is not a metaphor. The Getty already described cyanotype as an image with no layer of its own on the paper, not even baryta, the white layer other photographic papers have: the blue coats the fibers of the support itself2. What was missing was a close look, fiber by fiber, and a measurement of what was there.

The experiment#

Sawako Sentoku, Mari Kurashina and Keiko Kida work in the conservation science laboratory at Tokyo University of the Arts. They made cyanotypes with the traditional recipe on Whatman No. 1 cotton filter paper. They exposed them for 20 minutes under a black light lamp peaking at 368 nm and washed them for 20 minutes in distilled water1.

For comparison, they also made a print with half the light, another coated and washed without exposure, and a paper colored with artists’ Prussian blue pigment1. That last sample is the key to the study: Prussian blue as well, but laid on top of the paper instead of formed in it.

How the study looked at the blue of a cyanotype
Technique What it shows What it found Source
X-ray diffraction Which crystalline compound is present That the blue formed in the paper is Prussian blue 1
Optical microscopy The color in the fiber cross section Fibers blue inside in the cyanotype; not in the painted paper 1
Micro-Raman spectroscopy The carbon-nitrogen bond of the cyanide The signal, around 2150 cm−1, inside the cyanotype fiber 1
Scanning electron microscopy The particles one by one Particles on the surface and inside the fiber 1

The starting chemistry is the usual one: light reduces the iron(III) in the citrate to iron(II), which reacts with the ferricyanide and forms Prussian blue1. That pigment has no fixed formula: it contains iron(III), the hexacyanoferrate(II) anion and a variable amount of water1.

What they saw: blue inside the fiber#

In the cross sections, the more light a sample had received, the deeper into the thickness of the paper the blue fibers reached; in the unexposed sample no blue appeared1. Light doesn’t only color the side facing the sun: the more light the sheet gets, the deeper the blue forms.

The difference from the painted pigment was stark. In the colored paper, the particles, up to about 200 nm, sat on the surface of the fibers and in clumps, and the inside of the fiber was not blue. In the cyanotype, the fiber looked blue all the way through, as if dyed1. Spectroscopy confirmed the cyanide signal of Prussian blue inside those fibers1.

Painted pigment versus cyanotype: where the blue sits in the fiberTwo cross sections of a cotton fiber, with the central cavity (lumen) labeled. Left, paper colored with Prussian blue pigment: clumps of particles, up to about 200 nm, only around the outer edge; the inside stays white. Right, cyanotype: the whole cross section in blue, with fine particles of 20-100 nm on the surface and 20-50 nm inside the wall. Approximate scale bar: a cotton fiber is 12 to 20 µm wide. Note: diagram not to scale, with the particles greatly enlarged; data from Sentoku, Kurashina and Kida (2025).Paper colored with Prussian blue pigmentlumenparticles up to about 200 nm, on the surface and in clumpsthe inside of the fiber stays whiteCyanotypelumenthe whole cross section, in blue20-100 nm on the surface20-50 nm insidecotton fiber: 12-20 µm wide (approximate scale)Diagram not to scale; the particles are greatly enlarged. Data from Sentoku, Kurashina and Kida (2025). Painted pigment versus cyanotype: where the blue sits in the fiberPaper colored with Prussian blue pigmentlumenparticles up to about 200 nm, on the surface and inclumpsthe inside of the fiber stays whiteCyanotypelumenthe whole cross section, in blue20-100 nm on the surface20-50 nm insidecotton fiber: 12-20 µm wide(approx.)Diagram not to scale; the particles are greatlyenlarged. Data from Sentoku, Kurashina and Kida(2025).
Diagram 1Painted pigment versus cyanotype: where the blue sits in the fiber. When you paint with pigment, the blue stays outside the fiber; in a cyanotype, the fiber looks blue all the way through.

The electron microscope revealed the particles: about 20 to 100 nm on the fiber surface and 20 to 50 nm inside it1. To get a sense of scale, a cotton fiber is 12 to 20 µm wide, that is, between 12,000 and 20,000 nm1. The blue of a cyanotype is made of grains hundreds of times finer than the fiber that holds them.

The authors are cautious: they say it is possible that those particles are Prussian blue. And they consider it important for fixing the blue that the solution soaks into the fiber and forms the pigment there1. They don’t present it as a proven mechanism, and neither do we.

Particles that grow with light#

The particles were mostly round, with some cubic ones, and the square ones were plentiful in the sample that received the most light. The authors link this, as a possibility, to crystal growth from the greater exposure1. It’s a clue, not a conclusion.

What does this mean for washing a cyanotype?#

For washing a cyanotype, the study confirms what the water was already doing: carrying away the unreacted salts and leaving the blue anchored in the fiber. The only fixing a print needs is a good bath in running water3, and some of the blue is lost anyway, because its finest particles disperse in the water4.

If the blue lodges inside the fiber, what matters before exposure is that the solution gets into it. That is the point of wetting agents such as Tween 20, which help spread the solution evenly4, and of choosing a paper that absorbs well. Washing, step by step, is covered in developing a cyanotype.

And for preserving it?#

For preserving antique cyanotypes, the study gives one more reason not to clean them with water. Mike Ware advises against even a simple aqueous wash because of the risk of losing image, and Sentoku and her colleagues note that wet cleaning is usually not advisable for that reason5,1.

The authors add a caveat that matters to anyone working on fabric. If fixing depends on the solution soaking the fiber, the risk of image loss may be different on other supports, such as textiles or glass, where the image is held by a gelatin layer1. If you have an antique piece, the careful approach is in antique cyanotypes.

What is still unknown#

The study presents itself as a first step. Three questions remain open: why the particles inside are smaller than those on the surface, how they grow during the process and how, in the end, they become fixed1.

In the meantime, what we do know is that the blue forms inside the fiber, and that explains why a well-washed print holds together without a binder. The full chemistry of the process, from light to pigment, is in how cyanotype works. And more close-up looks are in The Journal.

More from the Journal

Your next step

Understand the full chemistry of the blueLight changes the iron in the citrate, and that iron forms Prussian blue with the ferricyanide. How cyanotype works, step by step, and why it’s blue.

Sources

  1. Sentoku, S., Kurashina, M. and Kida, K. (2025). Observation of blue particles formed by photosensitizing reaction on paper fibres of cyanotypes. Photochem, 5(3), Article 18. https://doi.org/10.3390/photochem5030018 12345678910111213141516171819
  2. Stulik, D. C. and Kaplan, A. (2013). Cyanotype. In The atlas of analytical signatures of photographic processes. Getty Conservation Institute. https://www.getty.edu/conservation/publications_resources/pdf_publications/pdf/atlas_cyanotype.pdf
  3. Image Permanence Institute. (n.d.). Cyanotype. Graphics Atlas. Rochester Institute of Technology. https://new.graphicsatlas.org/cyanotype Accessed October 17, 2026.
  4. Ware, M. (n.d.). The New Cyanotype process. Mike Ware: Alternative photography. https://www.mikeware.co.uk/mikeware/New_Cyanotype_Process.html Accessed October 16, 2026. 12
  5. Ware, M. (2003). A blueprint for conserving cyanotypes. Topics in Photographic Preservation, 10, 2-18. https://resources.culturalheritage.org/pmgtopics/2003-volume-ten/10_02_Ware.pdf

Reviewed on October 16, 2026. If you spot an error or a missing source, write to us and we’ll look into it.