In short
- The reference formula is Mike Ware’s: 25 g of green citrate and 10 g of ferricyanide.
- Each chemical is dissolved in distilled water to make 100 ml, and the two solutions are mixed in equal parts.
- The solutions are stored separately, in brown bottles and in the dark; the mix doesn’t last long.
- A 20.3 × 25.4 cm print takes about 1.5 ml of mix with a coating rod, and up to twice that with a brush.
- Recipes with a cited source use 20-26 g of citrate and 9-10 g of ferricyanide per 100 ml.
- Solution A is the citrate and B the ferricyanide, but the name on the label is what counts.
Safety: Wear safety glasses and nitrile gloves to mix and brush on the solution; if it splashes into your eyes, rinse with plenty of water for 15 minutes. More on safety
Safety: Work away from food and drink, with dedicated tools that never go back to the kitchen. More on safety
Materials list
Check off what you already have on the table. The “Amazon” links are affiliate links.
Your check marks are saved only in this browser. No account needed.
On this page (8 sections)
What liquid is used to make cyanotypes?#
The liquid used in cyanotype is the sensitizer solution: an equal-parts mix of two solutions of iron salts in distilled water, one of ferric ammonium citrate and one of potassium ferricyanide1. Spread on paper, it dries yellow; the blue only appears where light reaches it later2.
Why the mix works is explained in the chemistry of cyanotype. The Cyano Codex’s reference formula is the traditional one published by Mike Ware1:
Swipe to see more columns
| Solution | Chemical | Amount | Final volume | How to dissolve it |
|---|---|---|---|---|
| A | Ferric ammonium citrate, green form | 25 g | 100 ml | In about 70 ml of distilled water, at room temperature; then made up to 100 ml1 |
| B | Potassium ferricyanide | 10 g | 100 ml | In about 80 ml of distilled water, at room temperature; then made up to 100 ml1 |
| Mix | A and B in equal parts | — | 200 ml | Just before coating1 |
On this site, as in most recipes, Solution A is the citrate and Solution B is the ferricyanide. Some kits label the parts the other way around, so what counts is the name of the chemical on the label, not the letter.
The quantities are weight per final volume: 25 g of citrate in a solution that, once dissolved, measures 100 ml, not 25 g plus 100 ml of water1. The difference is small, but that’s why Ware first dissolves in less water and then makes it up to volume, that is, tops it up with water to the exact mark.
How to mix cyanotype solution#
Mixing cyanotype solution without a kit takes five steps: weigh, dissolve each chemical separately, label, store, and mix when you’re ready to use it. Before you open the bottles, review how to handle the chemicals safely and get the table ready, with everything from the materials list at hand.
Step 1: Weigh the two chemicals
Weigh 25 g of green ferric ammonium citrate and 10 g of potassium ferricyanide, each in its own beaker1. Use a scale and utensils set aside for the workshop that never go back to the kitchen, and wear nitrile gloves and safety goggles; how to choose them is covered in goggles and gloves for cyanotype.
Work under dim bulb light, away from the sun and from fluorescent lights: that’s how Ware prepares his sensitizer3, and the citrate is light-sensitive4.
How to tell it’s going well: the citrate is green and the ferricyanide red. If your “ferricyanide” is pale yellow, it’s ferrocyanide and won’t work for this formula5.
Safety: Weigh the powders slowly and away from drafts so you don’t raise dust; if the kit lets you dissolve them in their own bottle, even better. More on safety
Step 2: Dissolve the citrate: Solution A
Add the 25 g of citrate to about 70 ml of distilled water at room temperature and stir until it dissolves1. Then pour it into the graduated cylinder and top up with distilled water to 100 ml: this is called making up to volume, filling exactly to the mark. That way the concentration matches the recipe, 25 g per 100 ml of solution.
If you have doubts about the product, check what to look for on the label of ferric ammonium citrate: the green variety and the word “ammonium” are the two keys.
How to tell it’s going well: no undissolved powder is left at the bottom of the beaker.
Safety: Keep the powders and solutions away from light and heat, and never bring them near a flame: ferricyanide decomposes if heated strongly and gives off toxic gases. More on safety
Step 3: Dissolve the ferricyanide: Solution B
Wash and dry the graduated cylinder. Add the 10 g of ferricyanide to about 80 ml of distilled water, also at room temperature, stir until dissolved and make up to 100 ml1. The two solutions don’t meet until the last step, because the mix lasts much less time than each one on its own6.
If it’s your first time buying the chemical, check the color and CAS number on the potassium ferricyanide page.
How to tell it’s going well: no red crystals are left at the bottom of the beaker.
Safety: Wear safety glasses and nitrile gloves to mix and brush on the solution; if it splashes into your eyes, rinse with plenty of water for 15 minutes. More on safety
Step 4: Label and store the two solutions separately
Pour each solution into its own amber glass bottle, close it and label it right away with the chemical’s name, the concentration and the date; the cyanotype bottle labels have spaces for those. Mike Ware stores the stock solutions separately, in brown bottles and in the dark1. Kept separate, they last much longer than mixed: Jacquard states at least 6 months to 1 year for those in its kit6.
The citrate solution is the more delicate one, because it’s a good food for mold: within one or two weeks it can be covered with a thick layer1. How to extend its life and how to tell if it has gone bad is explained in how long cyanotype solution lasts.
How to tell it’s going well: each bottle says which chemical it contains, not just “A” or “B.”
Safety: Store chemicals and solutions tightly closed, labeled, in dark glass, away from acids and out of the reach of children. More on safety
Step 5: Mix in equal parts just before coating
Measure equal volumes of Solution A and Solution B and mix them in a clean beaker: that mix is the sensitizer1. Make only what you’ll use in the session, because the mix doesn’t last long: days, according to Ware1, and 2 to 4 hours, according to Jacquard’s instructions7.
To work out how much to mix, Ware estimates about 1.5 ml for a 20.3 × 25.4 cm print spread with a glass rod, and up to twice that with a brush1. On that basis, an A4 sheet takes about 1.8 ml with a rod and up to about 3.6 ml with a brush (our calculation). This figure doesn’t apply to fabric. For other formats, work out the mix with the Sensitizer Calculator.
How to tell it’s going well: once spread and dry, the coating is pale yellow; if the paper turns green or blue before exposure, it has fogged: it’s reacting without light and the whites will come out tinted3.
Safety: Keep leftover solution and the first wash bath in a closed, labeled container for your local hazardous waste collection point; later rinses can go down the drain with plenty of water. More on safety
With the mix ready, the next step is to spread it: we explain how in how to coat paper for cyanotype.
How long should the solution rest before use?#
Cyanotype solution doesn’t need to rest to mature. In Ware’s recipe, each chemical is dissolved at room temperature and the solutions are mixed when they’re about to be used1. The 24 hours you see quoted come from Jacquard: it’s how long its powder takes to dissolve fully in the kit bottle6.
If you mix loose chemicals, as on this page, the test is different: the solution is ready when nothing is left undissolved. If you use a powder set, follow its dissolving instructions and don’t confuse that waiting time with a chemical rest.
Distilled or tap water?#
To make up the solutions, use distilled water if you can: it’s what the reference formula calls for1. In an educational setting, Redden and Crawford accept tap water for mixing and rinsing8. For washing, tap water is fine if it isn’t hard or alkaline, because that kind of water degrades the image9.
The reason lies in the pigment. Prussian blue is stable in neutral or acidic conditions, but alkalis break it down10. Ware sets the limit for wash water at pH 7: nothing above that11. Hard water is water with a lot of calcium salts. If you know yours is hard, review developing cyanotypes before your first wash.
Why don’t cyanotype recipes agree?#
Cyanotype recipes don’t agree because ferric ammonium citrate has no fixed composition: its iron ranges from 14% to 28%12. Even so, those with a verified source fall within a narrow range: between 20 and 26 g of citrate and between 9 and 10 g of ferricyanide per 100 ml13.
Swipe to see more columns
| Source | Citrate per 100 ml | Ferricyanide per 100 ml | Mix | Note |
|---|---|---|---|---|
| Mike Ware, traditional formula (this site’s reference) | 25 g, green form | 10 g | 1:1 | In distilled water1 |
| National Science and Media Museum | 26 g, green form (6.5 g in 25 ml) | 9.2 g (2.3 g in 25 ml) | 1:1 | The per-100 ml conversion is our calculation13 |
| Jacquard, sensitizer in its kit | 20 % | 9 % | 1:1 | Doesn’t state whether the percentage is weight by volume or which form of citrate it uses14 |
| Sentoku et al. (2025), following Ware | With 0.6-0.7 mol/l of iron | 0.3 mol/l, about 9.9 g (our calculation) | 1:1 | Peer-reviewed lab study15 |
Moles per liter (mol/l) is the concentration measure chemists use: it counts molecules instead of grams. The ratio between the two chemicals ranges from about 2.2 to 2.8 parts citrate to one part ferricyanide (our calculation from the figures in the table), and Ware’s is 2.5. We haven’t found a source linking that ratio to print contrast, an idea that often circulates.
| What you’ll hear | What the sources say | Source |
|---|---|---|
| “Herschel’s original formula”: 20% citrate and 16% ferricyanide | Herschel gave no figures in 1842: he called for a “moderately concentrated” citrate solution that would dry yellow, not at all brown. We haven’t been able to confirm that 20% and 16% in reliable sources | 2 |
| Equal volumes of 8.1% ferricyanide and 20% citrate | We haven’t been able to confirm it in reliable sources: it doesn’t appear in Ware or in Herschel | 1 |
| 10% of each chemical, attributed to Christina Z. Anderson | We haven’t been able to consult the original work to confirm it, so we don’t give it | — |
| 20 g of citrate and 10 g of ferricyanide, attributed to the supplier George Weil | We haven’t located the original source | — |
| 25 g of citrate with 12 g or 15 g of ferricyanide | We haven’t found a verified source for those quantities | — |
| The solution has to rest for 24 hours | That’s the time Jacquard gives for its powder to dissolve fully in the bottle, not a chemical rest | 6 |
From scratch, a two-bottle set or ready-mixed?#
Making cyanotypes without a kit is exactly what this page explains: buying the two chemicals separately, weighing them and making up the solutions. The in-between option is a pre-weighed powdered chemistry set: you add water to each bottle and mix the two parts in equal amounts.
If you use a set, follow its dissolving instructions: Jacquard calls for 24 hours for the powder in its kit to dissolve fully6. Read the labels too, because some kits label parts A and B the other way around from this site.
Ready-mixed liquid chemistry saves all the work. We would only include it if the manufacturer states the composition and publishes its safety data sheet, and until we find one that does, we don’t include it. The types of kit, with what each one contains, are in cyanotype kits.
If something goes wrong#
| What you see | Most likely cause | What to do |
|---|---|---|
| The powder won’t fully dissolve | It needs more time or stirring | Stir more and wait, without heating; Jacquard gives 24 h for the powder in its kit6 |
| A layer of mold on the citrate solution | It’s a good food for mold, which can appear within one or two weeks1 | No source says whether it can be filtered and used again: test it on a strip before using it on a print |
| The paper turns green or blue before exposure | Chemical fog: the coating is reacting without light3 | Check the causes of fog in the whites before coating another sheet |
| The whites come out yellow after washing | Sensitizer is left in the paper: wash until the yellow is gone1 | See why my cyanotype comes out yellow |
| The blue comes out pale or washes away | Some of the “soluble” blue disperses in the wash9, and the print may be underexposed7 | See how to get a deeper blue |
Variations on the formula#
The most useful variation is a wetting agent, a product that helps the paper absorb the solution. Ware recommends adding one or two drops of Tween 20 (polysorbate 20) diluted to 20% per 10 ml of mix to the traditional formula1. Its safety data sheet doesn’t classify it as hazardous16, but it can react badly with gelatin-sized papers9.
Beyond the classic formula there are other chemistries, with other chemicals and a different risk profile. The best known is Mike Ware’s New Cyanotype, with ferric ammonium oxalate: we explain it in Ware’s New Cyanotype.
Frequently asked questions
Can I make a larger batch at once?
Yes, as long as you keep the proportions: 25 g of citrate per 100 ml of Solution A and 10 g of ferricyanide per 100 ml of Solution B. What you should make in small amounts is the mix, which doesn’t last long. The two solutions kept separate last much longer, so you can keep one bottle of each and mix at each session.
Can I use brown ferric ammonium citrate in this formula?
Yes. Mike Ware recommends the green form, but says the brown also works, though more slowly. If you use it, make the solution with the same amount and adjust the exposure time with a test strip, because the times that work with green won’t work as they are.
How much solution do I need for an A4 sheet?
Going by Mike Ware’s estimate, about 1.8 ml of mix if you spread it with a glass rod, and up to about 3.6 ml with a brush: this is our own calculation from his figures for 20.3 × 25.4 cm. It doesn’t apply to fabric, because fabric absorbs differently. Always make a little more than you need.
Which is Solution A and which is Solution B?
On this site, as in most recipes, A is the ferric ammonium citrate solution and B the potassium ferricyanide solution. Not every kit follows that convention and some label the parts the other way around. That’s why it’s worth labeling the bottles with the chemical’s name and not just the letter.
Your next step
Sources
- Ware, M. (n.d.). The traditional cyanotype process. Mike Ware: Alternative photography. https://mikeware.co.uk/mikeware/Traditional_Cyanotype.html Accessed October 16, 2026. 123456789101112131415161718192021
- Herschel, J. F. W. (1842). On the action of the rays of the solar spectrum on vegetable colours, and on some new photographic processes. Philosophical Transactions of the Royal Society of London, 132, 181-214. https://doi.org/10.1098/rstl.1842.0013 Cited: art. 212. 12
- Ware, M. (2009). New Cyanotype: Siderotype workshop notes. https://www.mikeware.co.uk/downloads/CyanoWork.pdf Accessed October 17, 2026. 123
- Thermo Scientific Chemicals. (n.d.). Ammonium iron(III) citrate, 16.5 to 18.5% Fe (AC211842500) [Product page]. Fisher Scientific. https://www.fishersci.com/shop/products/ammonium-iron-iii-citrate-16-5-18-5-fe-thermo-scientific/AC211842500 Accessed October 17, 2026.
- Sigma-Aldrich. (2026). Safety data sheet: Potassium hexacyanoferrate(II) trihydrate (version 6.12, product 455989). https://www.sigmaaldrich.com/sds/aldrich/455989. Accessed October 17, 2026.
- Jacquard Products. (n.d.). Cyanotype [Cyanotype Kit instruction booklet]. https://jacquardproducts.com/s/Cyanotype-Kit-INSTRUCTION-BOOKLET.pdf Accessed October 17, 2026. 123456
- Jacquard Products. (2021). Cyanotype detailed instructions [Manufacturer’s instructions, version 08.17.21]. https://cdn.shopify.com/s/files/1/0053/5540/5423/files/Cyanotype_Instructions.pdf Accessed October 16, 2026. 12
- Redden, H. and Crawford, A. (2025). Anna Atkins and the making of macroalgae cyanotypes and their role in science education. Applied Phycology, 6(1), 1-8. https://doi.org/10.1080/26388081.2024.2435049
- Ware, M. (n.d.). The New Cyanotype process. Mike Ware: Alternative photography. https://www.mikeware.co.uk/mikeware/New_Cyanotype_Process.html Accessed October 16, 2026. 123
- Stulik, D. C. and Kaplan, A. (2013). Cyanotype. In The atlas of analytical signatures of photographic processes. Getty Conservation Institute. https://www.getty.edu/conservation/publications_resources/pdf_publications/pdf/atlas_cyanotype.pdf
- Ware, M. (2022). Alternative photographic processes: Simple Cyanotype [PDF instructions]. https://mikeware.co.uk/downloads/SimpleCy22.pdf Accessed October 16, 2026.
- Ware, M. (n.d.). Towards an unproblematic cyanotype chemistry. Mike Ware: Alternative photography. https://mikeware.co.uk/mikeware/tocyan.html Accessed October 16, 2026.
- National Science and Media Museum. (2011, February 18). Introduction to the cyanotype process. National Science and Media Museum Blog. https://blog.scienceandmediamuseum.org.uk/introduction-cyanotype-process/ Accessed October 17, 2026. 12
- Jacquard Products. (2019). Cyanotype FAQs [Manufacturer’s document, version 02.08.19]. https://cdn.shopify.com/s/files/1/2714/2506/files/Cyanotype-FAQs.pdf Accessed October 17, 2026.
- Sentoku, S., Kurashina, M. and Kida, K. (2025). Observation of blue particles formed by photosensitizing reaction on paper fibres of cyanotypes. Photochem, 5(3), Article 18. https://doi.org/10.3390/photochem5030018
- AppliChem GmbH. (2025). Safety data sheet: Polysorbate 20 (version 6.14, art. A4974). https://pdf.dutscher.com/doc/348637/348637_FDSen.pdf. Accessed October 16, 2026.
Reviewed on October 16, 2026. If you spot an error or a missing source, write to us and we’ll look into it.
How to cite this page
The Cyano Codex. (2026, October 16). Cyanotype formula: how to mix the solution. https://cyanocodex.com/en/chemistry/formula/